I-Si-TPV 2250- 75A thermoplastic vulcanizate elastomer iwukuthinta okuthambile, i-thermoplastic silicone elastomer evumelana nesikhumba enikeza ukumelana nokuhunyazwa okukhethekile, ukumelana namakhemikhali, nokunamathela okuhle kakhulu ku-EVA namanye ama-polar substrates.
I-Si-TPV 2250- 75A ingasetshenziswa njengesilungisi se-eco-friendly, esisebenza kahle kakhulu se-thermoplastic elastomer esidizayinelwe izinhlelo zokusebenza ze-EVA ezinegwebu lamakhemikhali. Iletha ikhwalithi ephezulu yegwebu elinesakhiwo samaseli afanayo, ukunciphisa ukuncipha kokushisa okushisayo, kanye nokuzinza kwe-dimensional okuthuthukisiwe ngenkathi ivimbela ukufuduka kwamakhemikhali, ikwenze kube enye indlela enhle kakhulu yokufaka amagwebu ngokweqile. Izinto ezisetshenziswayo zikhiqiza amagwebu angasindi kakhulu, athambile, anwebekayo anokumelana okukhethekile nokugqoka/okushelelayo kanye nokufana kombala okungaguquki, okuholela ekukhiqizeni okuphezulu komkhiqizo. Ukucutshungulwa kwayo okuhle kakhulu kanye nokusebenza kahle kwezindleko kuyenza ifanelekele izicathulo, okokusebenza kwezemidlalo, izisetshenziswa zezokwelapha, nezinhlelo zokusebenza zokupakisha ezivikelayo, ezinikeza kokubili izinzuzo zokusebenza nokuzinza.
Elongation at Break | 80% | ISO37 |
Amandla Okuqina | 6.12Mpa | ISO37 |
Shore A Ukuqina | 75A | ISO868 |
Ukuminyana | 1.06 | ISO1183 |
Izinyembezi Amandla | 30.63kN/m | ISO34 |
I-Modulus ye-Elasticity | 10.26Mpa | ISO37 |
I-MI(190℃,10KG) | 5.54g/10min | ISO1133 |
Izimo | I-Si-TPV 2250-75A | iyunithi |
Isikhathi sokumisa | 2-4 | h |
Ukomisa izinga lokushisa | 80 | ℃ |
Izinga lokushisa le-Zone 1 | 120-140 | ℃ |
Izinga lokushisa le-Zone 2 | 140-160 | ℃ |
Izinga lokushisa le-Zone 3 | 140-170 | ℃ |
Izinga lokushisa le-Zone 4 | 170-175 | ℃ |
I-Nozzle noma izinga lokushisa lokufa | 175-185 | ℃ |
1. Imikhiqizo ye-elastomer ye-Si-TPV ingakhiqizwa kusetshenziswa izinqubo zokukhiqiza ezisezingeni eliphezulu ze-thermoplastic, okuhlanganisa ukugoqa ngokweqile noma ukubumba ngokuhlanganyela nama-substrates epulasitiki njenge-PC, i-PA.
2. Ukuzwakala okusilika okwedlulele kwe-Si-TPV elastomer akudingi ukucutshungulwa okwengeziwe noma izinyathelo zokumboza.
3. Izimo zenqubo zingahluka ngemishini ngayinye kanye nezinqubo.
4. I-desiccant desiccant dehumidifying drying inconywa kukho konke ukomisa.
25KG / isikhwama, isikhwama sephepha sobuciko esinesikhwama sangaphakathi se-PE.
Ezokuthutha njengamakhemikhali angeyona ingozi. Gcina endaweni epholile futhi enomoya omuhle.